24.70 g Epon 812
33.25 g Dodecenyl succinic anhydride
31.05 g Araldite 506
Mix well by stirring. Use disposable syringes to add:
2.3 ml Dibutylphthalate
2.5 ml DMP-30
Continue to mix well by stirring. Try to avoid incorporating excess air. If this occurs, resin may be degassed by subjecting it to a mild vacuum. Store resin in 10 ml syringes at -20°C.